Production Character:
1. Low processing temperature, 100℃ can be processed to produce wire, laminated glass film;
2. Thickness 0.1~0.5mm;
3. No black spots, no impurities;
Operation Procedure:
Sandwich film between two glasses, fix all corners with wood tape in case of displacement→Turn on vacuum pump for 5~10 minutes, make sure silicone bag no air left→Put into furnace, heating up to 60~65℃(glass surface), holding temperature 20~30 minutes→Go on heating up to 100~115℃(glass surface ), holding temperature 30 minutes →Cool down under 60℃(glass surface), then turn off vacuum pump→Open furnace,take out glass.